daohang fenxiangbox searchbox qikanlogonew daohangnew searchboxnew navrightzone footerzone paper

Research Progress on Fabrication of High-Purity Tantalum Targets for Advanced Process Chip AITranslate

1.School of Materials Science and Engineering,Zhejiang University,Hangzhou 310000,China
2.Konfoong Materials International Co.,Ltd.,Ningbo 315400,China
3.College of Chemical and Material Engineering,Quzhou University,Quzhou 324000,China
AITranslate
Publisher: Youke Publishing Co., Ltd
Share Citation Information Add to Favorites Download PDF

    Scan to share on WeChat or Moments

Use WeChat scan.
Share with WeChat friends or Moments

Abstract AITranslate

In integrated circuits with feature sizes below 90 nm,Cu interconnects has replaced Al as the new interconnect metal due to their advantages of lower resistivity,higher melting point,superior resistance to stress migration,and improved resistance to electromigration. When Cu was directly interconnected with Si in integrated circuits,it could lead to severe diffusion and generate interface thermal stress at above 120 ℃ and could result in the failure of wire electrical performance and the delamination of the interface. Therefore,it is necessary to incorporate Ta diffusion barrier layer between Cu and Si. Ta/TaN barrier layer effectively inhibited the diffusion of Cu and Si in high-temperature environments. On the other hand,it exhibits excellent adhesion to various layers and low contact resistance. Moreover,TaN demonstrated the ability to fill grain boundaries while maintaining a high level of thermal stability up to 650 ℃. These characteristics make Ta/TaN layer one of the optimal choices for constructing a diffusion barrier layer between Cu and Si. The preparation of the diffusion barrier layer Ta/TaN required the use of physical vapor deposition (PVD)techniques. However,the quality of the raw materials,particularly ultra-high purity Ta targets are used as a crucial material in PVD,could significantly affect the uniformity of the deposited film thickness and electrical performance due to issues such as purity,grain size,and texture gradient uniformity,this will have an impact on the yield of advanced process chips (sub-28 nm technology nodes). As integrated circuit chip fabrication technology advances to sub-28 nm technology nodes,the number of metal layers in logic circuits continues to increase,while the wire widths become increasingly narrow,and the requirements for barrier layer thickness also become thinner. In this review,it was crucial for ultra-high purity Ta targets to minimize texture and grain size variation gradients in order to achieve a more uniform distribution of the microstructure. However,Ta targets used in 130 and 90 nm processes would no longer meet the requirements of advanced process chips. The complete fabrication process for ultra-high purity Ta targets included the preparation of high-purity Ta powder,ingot casting,sintering,electron beam (EB)casting,forging,rolling,heat treatment,and machining. Both domestic and international Ta producers sourced the raw material for Ta products from Ta mines located in Africa and Australia. The raw material used for producing Ta powder was predominantly potassium tantalum fluoride (K2TaF7),and the acquisition of mineral resources was not considered challenging. Therefore,the key technology in the industrial chain of Ta targets for advanced process chips lay in the fabrication of target blanks that met the application requirements. The main focus and challenges within the complete fabrication process revolved around the purification of ultra-high purity Ta and the thermomechanical processing (TMP)of target blanks,which included forging,rolling,and recrystallization processes. Furthermore,it was essential to ensure the consistency of the microstructure among target blanks during mass production. The purification of Ta served as the starting point in the entire process,the most widely used method was the sodium reduction process using K2TaF7 as the raw material to produce high-purity Ta powder. Subsequently,the high-purity Ta powder was ingot formation and sintered in a vacuum furnace. The next step involved EB melting,which further purified the Ta and could achieve purities exceeding 99.999%(5N),meeting the application requirements for diffusion barrier layers in advanced process chips. However,due to the coarse grain size and uncontrolled crystal orientation of Ta obtained through EB melting,it could not be used without undergoing TMP. Thermal and multi-directional forging was beneficial for improving the uniformity of the microstructure and reducing texture gradients. For rolling,cross-rolling could eliminate the anisotropy generated by unidirectional rolling of Ta and ensure a more uniform distribution of texture on the rolled surface. Additionally,while cold rolling could more effectively achieve the desired texture,hot rolling activates more slip systems,resulting in smaller texture gradients. The rolling energy was retained within the Ta metal as stored energy and served as the driving force for recrystallization when the temperature increased during the recrystallization annealing stage. However,due to the different nucleation positions and mechanisms,the recrystallization rates of Ta in different regions of the target blanks vary,resulting in unavoidable texture gradients. Moreover,due to the high cost of ultra-high purity Ta and the high sensitivity of the later-stage processes to the preceding stages,the development of mature processes required significant investment,resulting in only a few companies worldwide having complete mastery of the entire fabrication process. This situation persisted despite the rapid development of the chip manufacturing industry. To further develop and optimize ultra-high purity Ta targets for integrated circuit applications and explore the use of Ta as a diffusion barrier layer in advanced process chips,three innovative research directions had been proposed:1)The sputtering lifetime of the 0.65-inch-thick Ta targets was increased by more than 3 times compared to the 0.25-inch targets. The increase in target thickness reduced the frequency of machine preventive maintenance (PM),and improved the utilization of expensive ultra-high purity Ta material,thereby reducing the cost of chip fabrication and enhancing economic efficiency. Therefore,it was necessary to redesign the ultra-high purity Ta TMP process to develop and optimize ultra-high lifetime,high thickness (0.65-inch)Ta targets that offer higher economic efficiency and material utilization rates. 2)By researching and improving the PVD process parameters of Ta targets,it was possible to fabricate α-Ta layers with enhanced diffusion barrier capabilities,thereby further improving the performance of advanced process chips. 3)Numerical simulations indicated that multiple passes of equal channel angular pressing refined the grain structure of tantalum,offering potential to improve the grain size and texture distribution of ultra-high-purity targets in advanced chip manufacturing.

KeyWords AITranslate

ultra-high purity tantalum sputtering target texture control very large-scale integration advanced process chip tantalum barrier layer material

[1]Murarka S P,Gutmann R J,Kaloyeros A E,Lanford W A. Advanced multilayer metallization schemes with copper as interconnection metal[J].Thin Solid Films,1993,236(1-2):257.

[2]汪凯,钟景明,李兆博,焦红忠,宿康宁,王莉,马小文.一种钽靶材织构评价方法的模型构建[J].材料开发与应用,2017,32(4):55

K Wang,J M Zhong,Z B Li,H Z Jiao,K N Su,L Wang,X W Ma. Model establishing of an evaluation method for tantalum target texture[J].Development and Application of Materials,2017,32(4):55.

[3]Hu C K,Liniger E G,Gignac L M,Bonilla G,Edelstein D. Materials and scaling effects on on-chip interconnect reliability[J].MRS Proceedings,2013,1559:701.

[4]Kuo Y L,Huang J J,Lin S T,Lee W H. Diffusion barrier properties of sputtered TaNx between Cu and Si using TaN as the target[J].Materials Chemistry and Physics,2003,80(3):690.

[5]陈秀华,王莉红,项金钟,吴兴惠,周桢来.超大规模集成电路铜布线扩散阻挡层TaN薄膜的制备研究[J].功能材料,2007,38(5):750.

X H Chen,L H Wang,J Z Xiang,X H Wu,Z L Zhou. Research on preparation of TaN diffusion barrier layer in ULSI (ultra large scale integration)Cu-metallization[J].Journal of Functional Materials,2007,38(5):750.

[6]Holloway K,Fryer P M,Cabral C,Harper J M E,Bailey P J,Kelleher K H. Tantalum as a diffusion barrier between copper and silicon:failure mechanism and effect of nitrogen additions[J].Journal of Applied Physics,1992,71(11):5433.

[7]Clevenger L A,Bojarczuk N A,Holloway K,Harper J M E,Cabral C,Schad R G,Cardone F,Stolt L. Comparison of high vacuum and ultra-high-vacuum tantalum diffusion barrier performance against copper penetration[J].Journal of Applied Physics,1993,73(1):300.

[8]梁海成,高博伦,王松伟,刘劲松,邓偲瀛.引线框架用高性能铜合金板带材及制备工艺[J].铜业工程,2024,(2):45.

H C Liang,B L Gao,S W Wang,J S Liu,S Y Deng. High-performance copper alloy plate strip for lead frame and reparation process[J].Copper Engineering,2024,(2):45.

[9]Christiansen C,Li B,Angyal M,Kane T,McGahay V,Wang Y Y,Yao S. Geometry,kinetics,and short length effects of electromigration in Mn doped Cu interconnects at the 32 nm technology node[A].2012 IEEE International Reliability Physics Symposium (IRPS)[C].Anaheim,USA:IEEE,2012. doi:10.1109/IRPS.2012.6241856.

[10]Hu C K,Gignac L,Rosenberg R. Electromigration of Cu/low dielectric constant interconnects[J].Microelectronics Reliability,2006,46(2-4):213.

[11]邵士英.集成电路中铜互连工艺浅谈[J].中国电子商务,2012,(7):99.

S Y Shao. Discussion on copper interconnection technology in integrated circuits[J].Chinese Electronic Commerce,2012,(7):99.

[12]陈海波,周继承,李幼真.集成电路Cu互连扩散阻挡层的研究进展[J].材料导报,2006,20(12):8.

H B Chen,J C Zhou,Y Z Li. Development of diffusion barrier for Cu interconnection in ULSI[J].Materials Review,2006,20(12):8.

[13]钟鑫生.解决90 nm及以下蚀刻中铜扩散的先进工艺[D].上海:复旦大学,2011. 28.

X S Zhong. The Advanced Process for Solving Copper Diffusion in 90 nm and Below Etching[D].Shanghai:Fudan University,2011. 28.

[14]郝国栋,田雪.钽微弧氧化电池负极制备及性能研究[J].稀有金属,2024,48(7):1050.

G D Hao,X Tian. Preparation and performance of tantalum micro-arc oxidation battery anode[J].Chinese Journal of Rare Metals,2024,48(7):1050.

[15]钟景明,何季麟,汪凯,李兆博,焦红忠,王莉.芯片用钽阻挡层材料织构控制技术研究[J].稀有金属,2018,42(12):1273.

J M Zhong,J L He,K Wang,Z B Li,H Z Jiao,L Wang. Texture control of tantalum barrier layer used for chips[J].Chinese Journal of Rare Metals,2018,42(12):1273.

[16]白宣羽,汪渊,徐可为,范多旺.集成电路的铜互连布线及其扩散阻挡层的研究进展[J].真空科学与技术快报,2004,24:78.

X Y Bai,Y Wang,K W Xu,D W Fan. Copper Interconnections and growth of diffusion barrier in integrated circuit fabrication[J].Journal of Vacuum Science and Technology (China),2004,24:78.

[17]袁倩靖.磁控溅射镀膜用纯钽靶材微观组织控制及其应用[D].哈尔滨:哈尔滨工业大学,2018. 4.

Q J Yuan. The Micro Structure Control and Application of Pure Tantalum Magnetron Sputtering Target[D].Harbin:Harbin Institute of Technology,2018. 4.

[18]潘文高,陈炜晔,吴澜尔.钽材轧制和再结晶织构演变研究进展[J].材料导报,2016,30(21):150.

W G Pan,W Y Chen,L E Wu. Progress in rolling and recrystallization textures of tantalum[J].Materials Review,2016,30(21):150.

[19]Michaluk C A. Correlating discrete orientation and grain size to the sputter deposition properties of tantalum[J]. Journal of Electronic Materials,2002,31(1):2.

[20]顾炜.铜互连中PVD Ta/TaN阻挡层的性能改进与缺陷控制研究[D].上海:上海交通大学,2007. 5.

W Gu. Study on Performance Improvement and Defect Control of PVD Ta/TaN Barrier Layer in Copper Interconnection[D].Shanghai:Shanghai Jiao Tong University,2007. 5.

[21]刘宁,杨辉,姚力军,王学泽,袁海军.集成电路用大尺寸高纯钽靶材的制备工艺进展[J].集成电路应用,2018,35(2):24.

N Liu,H Yang,L J Yao,X Z Wang,H J Yuan. The progresses on fabrication of large size high-purity tantalum targets for integrated circuits[J].Application of IC,2018,35(2):24.

[22]柴立元,钟海云.氟钽酸钾钠还原生产钽粉的工艺现状及展望[J].稀有金属与硬质合金,1994,(4):30.

L Y Chai,H Y Zhong. Present situation and prospect of technology of K2TaF7 sodium reduction for Ta powder production[J].Rare Metals and Cemented Carbides,1994,(4):30.

[23]何季麟,张学清,杨国启,郑爱国.电容器级钽粉关键技术与开发研究[J].中国材料进展,2014,33(9):545.

J L He,X Q Zhang,G Q Yang,A G Zheng. The key technique and R&D of capacitor grade tantalum powder[J].Materials China,2014,33(9):545.

[24]李仲香,杨国启,陈学清,程越伟,李慧,张健康.溅射钽靶材用高纯钽粉工艺研究[J].材料开发与应用,2017,32(3):67.

Z X Li,G Q Yang,X Q Chen,Y W Cheng,H Li,J K Zhang. Study on production process of high pure tantalum powder for tantalum target[J].Development and Application of Materials,2017,32(3):67.

[25]任志东,白掌军,李树荣,张学林.真空电子束熔炼制备超高纯钽锭工艺研究[J].湖南有色金属,2020,36(6):53.

Z D Ren,Z J Bai,S R Li,X L Zhang. The study of ultra-high purity tantalum ingot preparation by vacuum electron beam melting[J].Hunan Nonferrous Metals,2020,36(6):53.

[26]尚再艳,张涛,陈明,朱晓光,刘红宾,何金江.镍的电子束熔炼提纯研究[J].稀有金属,2013,37(1):116.

Z Y Shang,T Zhang,M Chen,X G Zhu,H B Liu,J J He. Purification of nickel ingot prepared by electron beam melting[J].Chinese Journal of Rare Metals,2013,37(1):116.

[27]刘业.电子束熔炼法提纯钨过程中杂质的去除工艺及其机理研究[D].长沙:中南大学,2013. 56.

Y Liu. Study of the Removal Technology and Mechanism of Impurities in Tungsten by Electron Beam Melting[D].Changsha:Central South University,2013. 56.

[28]魏忠梅,杨明杰,李麦海.冷压-轧制工艺对钽板组织与性能的影响[J].稀有金属与硬质合金,2000,(3):14.

Z M Wei,M J Yang,M H Li. Influence of cold pressing-rolling process on the structure and properties of Ta Slabs[J].Rare Metals and Cemented Carbides,2000,(3):14.

[29]邓超,刘施峰,姬静利,郝晓博,梁延祥.变形区形状参数对钽板组织均匀性的影响[J].稀有金属材料与工程,2014,43(8):2017.

C Deng,S F Liu,J L Ji,X B Hao,Y X Liang. Influence of roll gap geometry on through-thickness uniformity of texture and microstructure in clock-rolled tantalum[J].Rare Metal Materials and Engineering,2014,43(8):2017.

[30]郝晓博.高纯钽板冷轧及退火过程中微结构演变规律的研究[D].重庆:重庆大学,2015. 13.

X B Hao. Research on the Microstructure Evolution of High Purity Tantalum Plate During Cold Rolling and Subsequent Annealing Process[D].Chongqing:Chongqing University,2015. 13.

[31]Raabe D,Schlenkert G,Weisshaupt H,Lücke K. Texture and microstructure of rolled and annealed tantalum[J].Materials Science and Technology,1994,10(4):299.

[32]冯天,孔见,张勇,赵永好.轧制压下率、 路径对NiCoCr合金微观结构和力学性能的影响[J].有色金属科学与工程,2024,15(2):212.

T Feng,J Kong,Y Zhang,Y H Zhao. The effects of cold rolling thickness reduction and path on the microstructure and mechanical properties of NiCoCr alloy[J].Nonferrous Metals Science and Engineering,2024,15(2):212.

[33]毛宇成,刘施峰,范海洋,刘庆.高纯钽交叉轧制过程中微观结构和织构梯度的演变[J].电子显微学报,2017,36(1):7.

Y C Mao,S F Liu,H Y Fan,Q Liu. Evolution of texture gradient and microstructure of high purity tantalum in clock-rolling process[J].Journal of Chinese Electron Microscopy Society,2017,36(1):7.

[34]林男,刘施峰,柳亚辉,范海洋,祝佳林,邓超.高纯钽板异步轧制及后续退火过程中微观组织及织构演变研究[J].电子显微学报,2018,37(4):332.

N Lin,S F Liu,Y H Liu,H Y Fan,J L Zhu,C Deng. Study on microstructure and texture evolution during asymmetrical rolling and subsequent annealing of high pure tantalum plate[J].Journal of Chinese Electron Microscopy Society,2018,37(4):332.

[35]张行健,王志法,陈德欣,张瑾瑾.冷变形量及退火温度对钽板再结晶组织的影响[J].稀有金属与硬质合金,2005,(4):8.

X J Zhang,Z F Wang,D X Chen,J J Zhang. Effect of Deformation and annealing temperature on the microstructure of tantalum plate[J].Rare Metals and Cemented Carbides,2005,(4):8.

[36]柳亚辉,刘施峰,范海洋,刘庆.高纯钽板中晶粒生长的取向相关性研究[J].电子显微学报,2016,35(1):17.

Y H Liu,S F Liu,H Y Fan,Q Liu. Study on the orientation-dependent grain growth of high purity tantalum[J].Journal of Chinese Electron Microscopy Society,2016,35(1):17.

[37]Sandim H,Martins J P,Pinto A L. Recrystallization of oligocrystalline tantalum deformed by cold rolling[J].Materials Science and Engineering A Structural Materials,2005,392(1-2):209.

[38]祝佳林,刘施峰,柳亚辉,姬静利,李丽娟.冷轧高纯钽板退火过程中微观组织及织构演变的梯度效应[J].材料导报,2018,32(20):3595.

J L Zhu,S F Liu,Y H Liu,J L Ji,L J Li. Gradient of microstructure and texture evolution of cold rolled high purity tantalum plate during annealing process[J].Materials Review,2018,32(20):3595.

[39]Mathaudhu S N,Hartwig K T. Grain refinement and recrystallization of heavily worked tantalum[J].Materials Science and Engineering A,2006,426(1-2):128.

[40]陈勇棠,张伶俐.全球精密锻造技术专利布局与发展态势[J].锻压技术,2024,49(4):15.

Y T Chen,L L Zhang. Patent layout and development trend on global precision forging technology[J]. Forging & Stamping Technology,2024,49(4):15.

[41]杨西荣,戴炎,刘晓燕,罗雷,王敬忠,杨博海.纯钽等通道转角挤压织构演变数值模拟研究[J].塑性工程学报,2024,31(12):1.

X R Yang,Y Dai,X Y Liu,L Luo,J Z Wang,B H Yang. Numerical simulation study on texture evolution of pure tantalum during equal channel angular pressing[J].Journal of Plasticity Engineering,2024,31(12):1.

Basic Information:

DOI:10.13373/j.cnki.cjrm.XY23040019

Chinese Library Classification Number:TG146.4+16

Citation Information:

In integrated circuits with feature sizes below 90 nm,Cu interconnects has replaced Al as the new interconnect metal due to their advantages of lower resistivity,higher melting point,superior resistance to stress migration,and improved resistance to electromigration. When Cu was directly interconnected with Si in integrated circuits,it could lead to severe diffusion and generate interface thermal stress at above 120 ℃ and could result in the failure of wire electrical performance and the delamination of the interface. Therefore,it is necessary to incorporate Ta diffusion barrier layer between Cu and Si. Ta/TaN barrier layer effectively inhibited the diffusion of Cu and Si in high-temperature environments. On the other hand,it exhibits excellent adhesion to various layers and low contact resistance. Moreover,TaN demonstrated the ability to fill grain boundaries while maintaining a high level of thermal stability up to 650 ℃. These characteristics make Ta/TaN layer one of the optimal choices for constructing a diffusion barrier layer between Cu and Si. The preparation of the diffusion barrier layer Ta/TaN required the use of physical vapor deposition (PVD)techniques. However,the quality of the raw materials,particularly ultra-high purity Ta targets are used as a crucial material in PVD,could significantly affect the uniformity of the deposited film thickness and electrical performance due to issues such as purity,grain size,and texture gradient uniformity,this will have an impact on the yield of advanced process chips (sub-28 nm technology nodes). As integrated circuit chip fabrication technology advances to sub-28 nm technology nodes,the number of metal layers in logic circuits continues to increase,while the wire widths become increasingly narrow,and the requirements for barrier layer thickness also become thinner. In this review,it was crucial for ultra-high purity Ta targets to minimize texture and grain size variation gradients in order to achieve a more uniform distribution of the microstructure. However,Ta targets used in 130 and 90 nm processes would no longer meet the requirements of advanced process chips. The complete fabrication process for ultra-high purity Ta targets included the preparation of high-purity Ta powder,ingot casting,sintering,electron beam (EB)casting,forging,rolling,heat treatment,and machining. Both domestic and international Ta producers sourced the raw material for Ta products from Ta mines located in Africa and Australia. The raw material used for producing Ta powder was predominantly potassium tantalum fluoride (K2TaF7),and the acquisition of mineral resources was not considered challenging. Therefore,the key technology in the industrial chain of Ta targets for advanced process chips lay in the fabrication of target blanks that met the application requirements. The main focus and challenges within the complete fabrication process revolved around the purification of ultra-high purity Ta and the thermomechanical processing (TMP)of target blanks,which included forging,rolling,and recrystallization processes. Furthermore,it was essential to ensure the consistency of the microstructure among target blanks during mass production. The purification of Ta served as the starting point in the entire process,the most widely used method was the sodium reduction process using K2TaF7 as the raw material to produce high-purity Ta powder. Subsequently,the high-purity Ta powder was ingot formation and sintered in a vacuum furnace. The next step involved EB melting,which further purified the Ta and could achieve purities exceeding 99.999%(5N),meeting the application requirements for diffusion barrier layers in advanced process chips. However,due to the coarse grain size and uncontrolled crystal orientation of Ta obtained through EB melting,it could not be used without undergoing TMP. Thermal and multi-directional forging was beneficial for improving the uniformity of the microstructure and reducing texture gradients. For rolling,cross-rolling could eliminate the anisotropy generated by unidirectional rolling of Ta and ensure a more uniform distribution of texture on the rolled surface. Additionally,while cold rolling could more effectively achieve the desired texture,hot rolling activates more slip systems,resulting in smaller texture gradients. The rolling energy was retained within the Ta metal as stored energy and served as the driving force for recrystallization when the temperature increased during the recrystallization annealing stage. However,due to the different nucleation positions and mechanisms,the recrystallization rates of Ta in different regions of the target blanks vary,resulting in unavoidable texture gradients. Moreover,due to the high cost of ultra-high purity Ta and the high sensitivity of the later-stage processes to the preceding stages,the development of mature processes required significant investment,resulting in only a few companies worldwide having complete mastery of the entire fabrication process. This situation persisted despite the rapid development of the chip manufacturing industry. To further develop and optimize ultra-high purity Ta targets for integrated circuit applications and explore the use of Ta as a diffusion barrier layer in advanced process chips,three innovative research directions had been proposed:1)The sputtering lifetime of the 0.65-inch-thick Ta targets was increased by more than 3 times compared to the 0.25-inch targets. The increase in target thickness reduced the frequency of machine preventive maintenance (PM),and improved the utilization of expensive ultra-high purity Ta material,thereby reducing the cost of chip fabrication and enhancing economic efficiency. Therefore,it was necessary to redesign the ultra-high purity Ta TMP process to develop and optimize ultra-high lifetime,high thickness (0.65-inch)Ta targets that offer higher economic efficiency and material utilization rates. 2)By researching and improving the PVD process parameters of Ta targets,it was possible to fabricate α-Ta layers with enhanced diffusion barrier capabilities,thereby further improving the performance of advanced process chips. 3)Numerical simulations indicated that multiple passes of equal channel angular pressing refined the grain structure of tantalum,offering potential to improve the grain size and texture distribution of ultra-high-purity targets in advanced chip manufacturing.

quote

GB/T 7714-2015 [1] Qitao Huang, Lijun Yao, Weihua Zhong, et al. Research Progress on Fabrication of High-Purity Tantalum Targets for Advanced Process Chip[J]. Chinese Journal of Rare Metals, 2025, 49(5): 669-678. DOI:10.13373/j.cnki.cjrm.XY23040019.
MLA [1] Qitao Huang, et al., "Research Progress on Fabrication of High-Purity Tantalum Targets for Advanced Process Chip." Chinese Journal of Rare Metals, vol. 49, no. 5, 2025, pp. 669-678, https://doi.org/10.13373/j.cnki.cjrm.XY23040019.
APA [1] Qitao Huang, Lijun Yao, Weihua Zhong, Qianjing Yuan, Yanfang Wu, & Hui Yang. (2025). Research Progress on Fabrication of High-Purity Tantalum Targets for Advanced Process Chip. Chinese Journal of Rare Metals, 49(5), 669-678. https://doi.org/10.13373/j.cnki.cjrm.XY23040019
IEEE [1] Qitao Huang, Lijun Yao, Weihua Zhong, Qianjing Yuan, Yanfang Wu, and Hui Yang, "Research Progress on Fabrication of High-Purity Tantalum Targets for Advanced Process Chip," Chinese Journal of Rare Metals, vol. 49, no. 5, pp. 669-678, 2025, doi: 10.13373/j.cnki.cjrm.XY23040019. keywords: {ultra-high purity tantalum;sputtering target;texture control;very large-scale integration;advanced process chip;tantalum barrier layer material}